Saturday, 21 November 2026

Charlie's Shed - zinc plating

After a few experiments with electrolytic cleaning, the logical next step is to try some home plating again. Rooting about in the workshop I was pleased to discover that I had all the bits from the Gateros zinc plating kit I bought, maybe 12 years ago. 

However, this first experiment is a cheap supermarket option - the electrolyte is a mixture of white vinegar, tap water and table salt and the anodes are old, used zinc plates from Gateros.

My intention was to run at something like 0.06 A per square inch of work, which worked out to something like 0.24 A. This proved to be very slow indeed and I turned the current up a little bit.

My starting point was the same spanner that I used for the electrolytic cleaning, with some additional cleaning up from some 180 grit Scotchbrite.

After an hour also in the plating bath we came up with this:

You have to polish up the zinc as it comes from the bath but this is certainly plated all over and looks quite good, but I have learnt that rust, even converted rust is not a good basis for plating - you have to get down to bare steel.

 There's a few bits of the FH that will need zinc plating. Let's start with the rear wheel spindle:


Maybe not. Looks like we will need a bit of work to get these two back to the 1.2" AF they are supposed to have (that's for 11/16" CEI, by the way); as a matter of note, the drive side spindle uses a 11/16" washer and the brake side uses a 1" washer. 

Maybe the brake drum spacer is a better option, especially now we have some new anodes:


That came out rather well!



No comments:

Post a Comment